Skip to Content
Merck
HomeQuantitative mechanical characterization of TissueFab® bioinks during thermal gelation and 405 nm photocrosslinking with ElastoSens™ Bio

Quantitative mechanical characterization of TissueFab® bioinks during thermal gelation and 405 nm photocrosslinking with ElastoSens™ Bio

Application specialist: Dimitria B. Camasao, PhD

This study was conducted in collaboration between Rheolution (Quebec, Canada) and Merck Brazil (São Paulo, Brazil).

Abstract

This application note provides quantitative mechanical context for key steps in the recommended TissueFab® bioprinting protocol, connecting bioink preparation and thermal conditioning through printing and photocrosslinking to the mechanical properties of the final construct. ElastoSens™ Bio was used to quantify the mechanical transitions associated with thermal conditioning and 405 nm photocrosslinking of three TissueFab® bioinks. The formulations exhibited distinct thermal gelation kinetics and post-crosslinking stiffnesses, demonstrating that bioink selection influences the mechanical outcome of the printing workflow. Light intensity and exposure duration also strongly affected the final shear storage modulus (G′), providing quantitative guidance for adapting photocrosslinking conditions to achieve the desired construct mechanics.  

Section overview

Introduction

Successful extrusion-based 3D bioprinting requires a bioink to transition through different mechanical states: fluid enough for preparation and cartridge loading, sufficiently structured for controlled extrusion, and mechanically stable after printing. The recommended protocol provided by Merck for TissueFab® bioinks offers a practical baseline for this sequence, including warming the bioink to 37 °C for handling, cooling the loaded cartridge to 15-20 °C to induce gelation before printing, and exposing the printed construct to 405 nm visible light for photocrosslinking. While these steps define the practical workflow, quantitative mechanical information can help users understand how quickly the bioink gels during cooling and how photocrosslinking conditions affect the final construct stiffness. These transitions can be monitored through the shear storage modulus (G′), which reflects the elastic response, and tan δ (G″/G′), which describes the balance between viscous and elastic behavior.

In this collaborative study between Merck and Rheolution, ElastoSens™ Bio was used to monitor TissueFab® bioinks in real time during thermal gelation and visible-light photocrosslinking. The experimental design reproduces key transitions of the recommended bioprinting workflow, providing quantitative mechanical information to support process understanding and optimization.

Materials and methods

Study design

Three bioink formulations, TissueFab® GelMA-Conductive-Vis (915963), TissueFab® GelMA-Bone-Vis (915033), and TissueFab® GelMA-Vis (918741), were characterized with ElastoSens™ Bio following an experimental sequence designed to reproduce the key steps of their bioprinting protocol. Samples first underwent thermal gelation without light exposure, while G′ and tan δ were monitored continuously. At 40 min, the samples were photocrosslinked with 405 nm light for 15 s at 100% intensity, and measurements were continued to quantify the resulting increase in stiffness. Thermal gelation time was determined from the characteristic maximum in tan δ, while plateau G′ was calculated as the average over the 65-70 min interval. To evaluate the influence of photocrosslinking settings, TissueFab® GelMA-Bone-Vis was tested at different light intensities with a fixed exposure duration of 15 s, while TissueFab® GelMA-Vis was tested at different exposure durations at 100% light intensity.

Photographs of three TissueFab™ bioinks: (A) GelMA-Vis, (B) GelMA-Bone-Vis, and (C) GelMA-Conductive-Vis. Top panels show the bioink samples in ElastoSens™ Bio sample holders during testing, while bottom panels show the corresponding samples after removal from the holders.

Representative TissueFab® bioink samples during ElastoSens™ Bio testing (top) and after removal from the sample holders (bottom). a) TissueFab® GelMA-Vis, b) TissueFab® GelMA-Bone-Vis, c) TissueFab® GelMA-Conductive-Vis.

Results and discussion

Effect of thermal gelation and photocrosslinking on the mechanical properties of TissueFab® bioinks

The evolution of G′ and tan δ during the first 40 min at 20 °C revealed clear differences in thermal gelation among the three TissueFab® formulations (Figure 1), reflecting the cartridge-cooling step performed before printing. As the bioinks progressively developed a more elastic, solid-like structure, the peak in tan δ was used to identify the thermal gelation time. This occurred at approximately 6.5 min for TissueFab® GelMA-Conductive-Vis, 10.3 min for TissueFab® GelMA-Bone-Vis, and 10.4 min for TissueFab® GelMA-Vis.

At 40 min, the samples were exposed to 405 nm light for 15 s at 100% intensity (30 mW/cm²), representing the post-deposition stabilization step. All three formulations showed a rapid increase in G′ following illumination (Figure 1), quantifying the mechanical reinforcement produced by photocrosslinking. The magnitude of this response depended strongly on formulation: TissueFab® GelMA-Conductive-Vis reached the highest plateau G′ at approximately 24.0 kPa, followed by TissueFab® GelMA-Bone-Vis at approximately 19.2 kPa and TissueFab® GelMA-Vis at approximately 8.3 kPa. These results demonstrate that identical photocrosslinking conditions can produce substantially different final stiffnesses, highlighting bioink formulation as an important determinant of the mechanical properties of the resulting constructs.

Overall, the thermal gelation and photocrosslinking results indicate that the incorporation of additives influences both gelation kinetics and the resulting mechanical properties. In particular, TissueFab® GelMA-Bone-Vis and TissueFab® GelMA-Conductive-Vis contain hydroxyapatite and carbon nanotubes, respectively, which may contribute to the increased stiffness observed in these formulations.

Rheological characterization of three TissueFab™ bioinks (GelMA-Conductive-Vis, GelMA-Bone-Vis, and GelMA-Vis) showing changes in shear storage modulus (G′) and tan δ during thermal gelation at 20 °C and subsequent photocrosslinking with 405 nm light for 15 s at 100% intensity. Bar graphs compare thermal gelation time and plateau storage modulus after photocrosslinking.

Figure 1.Quantification of thermal gelation and photocrosslinking during the TissueFab® bioprinting workflow. Evolution of the shear storage modulus (G′) and tan δ for TissueFab® GelMA-Conductive-Vis, TissueFab® GelMA-Bone-Vis, and TissueFab® GelMA-Vis (n = 3). Samples first underwent thermal gelation at 20 °C, representing the pre-print cooling and conditioning stage, followed by photocrosslinking at 40 min with 405 nm light for 15 s at 100% intensity (30 mW/cm²). The right panels summarize the thermal gelation time, determined from the characteristic maximum in tan δ, and the plateau shear storage modulus (G′) following photocrosslinking.

Effect of light intensity on post-photocrosslinking stiffness of TissueFab® bioinks

The Merck workflow instructs users to photocrosslink the printed construct with 405 nm visible light and to adapt the distance and exposure duration to the available light source. This makes the delivered light intensity an important processing variable. To quantify its effect, light intensity was varied while the wavelength and exposure duration were maintained constant.

To evaluate the effect of light intensity, TissueFab® GelMA-Bone-Vis samples were photocrosslinked for 15 s at 25%, 50%, and 100% intensity, corresponding to approximately 8, 15, and 30 mW/cm², respectively (Figure 2). Before light exposure, the G′ curves showed similar behavior during thermal gelation. However, following illumination at 40 min, a clear intensity-dependent response was observed, with G′ reaching approximately 3.5 kPa at 25% intensity, 9.7 kPa at 50% intensity, and 19.2 kPa at 100% intensity. These results demonstrate that increasing light intensity progressively increases the post-crosslinking stiffness of TissueFab® GelMA-Bone-Vis over the tested range.

Therefore, transferring a printing protocol between instruments should account for the actual irradiance delivered to the construct rather than relying on exposure duration alone.

Effect of 405 nm light irradiance on the shear storage modulus (G′) of TissueFab™ GelMA-Bone-Vis bioink following thermal gelation at 20 °C. Photocrosslinking for 15 s at irradiances of 8, 15, and 30 mW/cm² (25%, 50%, and 100% intensity, respectively) resulted in increasing plateau storage modulus with increasing light intensity.

Figure 2.Effect of 405 nm light irradiance on the mechanical stabilization of TissueFab® GelMA-Bone-Vis bioink (n = 1). Following thermal gelation at 20 °C, samples were exposed to 405 nm light for 15 s at irradiances of 8, 15, and 30 mW/cm², corresponding to 25%, 50%, and 100% light intensity, respectively. The resulting increase in the shear storage modulus (G′) with increasing irradiance demonstrates the effect of light-source setting on the mechanics of the final printed construct.

Effect of photocrosslinking duration on the post-crosslinking stiffness of TissueFab® bioink

The Merck protocol also identifies exposure duration as a parameter that may need to be adapted to the available light source and printing configuration. The effect of this parameter was therefore quantified using TissueFab® GelMA-Vis (Figure 3).

Samples were photocrosslinked with 405 nm light at 100% intensity for 15, 30, and 60 s. While the G′ curves showed similar behavior before photocrosslinking, clear differences emerged following light exposure. The plateau G′ values reached approximately 8.3, 17.3, and 21.5 kPa after 15, 30, and 60 s of exposure, respectively. The increase was particularly pronounced between 15 and 30 s, demonstrating that exposure duration strongly influences post-crosslinking stiffness and that changes in this parameter can substantially modify the mechanical properties of the photocrosslinked bioink.

Effect of 405 nm light exposure duration on the shear storage modulus (G′) of TissueFab™ GelMA-Vis bioink following thermal gelation at 20 °C. Photocrosslinking at 100% intensity (30 mW/cm²) for 15, 30, and 60 s resulted in progressively higher plateau storage modulus with increasing exposure duration.

Figure 3.Effect of 405 nm light exposure duration on the post-photocrosslinking stiffness of TissueFab® GelMA-Vis bioink (n = 1). Following thermal gelation at 20 °C, samples were exposed to 405 nm light at 100% intensity (30 mW/cm²) for 15, 30, or 60 s. Increasing exposure duration resulted in progressively higher shear storage modulus (G′), demonstrating the sensitivity of final construct stiffness to the duration selected for the post-print crosslinking step.

Together with the light-intensity experiment, these results highlight photocrosslinking as a critical processing step in the bioprinting workflow, since changes in irradiance, exposure duration, and source-to-construct distance can alter the effective light dose and substantially affect the final construct mechanics. This is particularly important when transferring protocols between bioprinters or external light sources, where direct mechanical characterization can help determine whether adapted crosslinking conditions achieve the desired mechanical endpoint.

Conclusion

The TissueFab® protocol provides users with the practical sequence required to prepare, print, and crosslink these bioinks. The present study complements this workflow by quantifying the mechanical changes associated with two critical transitions: thermal gelation before extrusion and photocrosslinking after deposition.

The three tested formulations displayed distinct thermal gelation behavior and substantially different mechanical properties after photocrosslinking. Under identical exposure conditions of 405 nm, 15 s, and 100% intensity, TissueFab® GelMA-Conductive-Vis produced the highest plateau G′, followed by TissueFab® GelMA-Bone-Vis, while TissueFab® GelMA-Vis produced the lowest stiffness.

However, the experiments further demonstrated that the resulting stiffness is not determined solely by bioink formulation, as processing parameters also influence the mechanical outcome. For TissueFab® GelMA-Bone-Vis, increasing light intensity from 25% to 100% resulted in a progressive increase in G′. Similarly, increasing the exposure duration of TissueFab® GelMA-Vis from 15 to 60 s substantially increased its post-crosslinking stiffness.

Overall, the mechanical outcome of the bioprinting workflow is influenced by both bioink formulation and processing conditions. Formulation affects thermal gelation and post-crosslinking stiffness, while light intensity and exposure duration provide additional control over the mechanical properties of the photocrosslinked bioink. By quantitatively linking thermal conditioning and photocrosslinking parameters to material properties, these measurements can support process optimization, method transfer, and more reproducible fabrication of 3D constructs.

Practical takeaways for the bioprinting workflow

  • Preparation: Warming the bioink makes it fluid for mixing and cartridge loading, followed by a deliberate cooling step before extrusion.
  • Pre-print conditioning: Thermal gelation is measurable and formulation-dependent, providing quantitative context for the cartridge-cooling step used to establish a print-ready material structure.
  • Printing: The thermally conditioned state precedes extrusion and helps connect temperature control with printing fidelity and shape retention.
  • Post-print stabilization: 405 nm photocrosslinking produces a rapid increase in G′, converting the deposited material into a mechanically stronger construct.
  • Light-source settings matter: Changes in irradiance or exposure duration can substantially affect the final G′, supporting the protocol recommendation to adapt crosslinking parameters to the available light source and configuration.
  • Formulation matters: Identical processing conditions can generate different mechanical endpoints for different TissueFab® bioinks. Knowing the final construct application and desired mechanical properties is essential for selecting the right bioink product.
  • Quantitative characterization complements the protocol: Real-time viscoelastic measurements can help users connect practical processing settings with the mechanical state of the material before and after printing.

Note: ElastoSens™ Bio is a trademark of Rheolution (Rheolution Inc.)

Related products

Loading